# ECSA calculator: double-layer capacitance, ECSA and roughness factor

> ECSA from double-layer capacitance: Cdl is the slope of Δi/2 against scan rate, ECSA = Cdl/Cs (0.040 mF/cm² in 1 M NaOH), and the roughness factor. Free.

URL: https://www.labcanvas.com/tools/ecsa-calculator

The electrochemically active surface area (ECSA) is the double-layer capacitance Cdl divided by a specific capacitance Cs: ECSA = Cdl/Cs. Record CVs at several scan rates in a potential window with no Faradaic current, read the anodic and cathodic current at one potential, and plot half their difference, Δi/2, against the scan rate: the slope is Cdl. McCrory et al. (2013) used Cs = 0.040 mF/cm² in 1 M NaOH and 0.035 mF/cm² in 1 M H₂SO₄, so Cdl = 0.1428 mF gives an ECSA of 3.57 cm² in alkaline solution; divided by the geometric area, 0.196 cm², that is a roughness factor of 18.2.

## Quick answer

- **What it does:** Fits the double-layer charging current against the scan rate to get Cdl, then gives the ECSA, the roughness factor and the specific ECSA for the specific capacitance you choose.
- **Formula:** i = Cdl·ν, so Cdl = slope of Δi/2 = (ia − ic)/2 against ν;  ECSA = Cdl/Cs;  RF = ECSA/A_geo
- **Example:** Charging currents at 10–100 mV/s give a Δi/2 slope of Cdl = 0.1428 mF; with Cs = 0.040 mF/cm² (1 M NaOH), ECSA = 0.1428/0.040 = 3.57 cm², and on a 0.196 cm² disc the roughness factor is 18.2.

Free, in the browser, no account needed. Updated 2026-11-23.

## Features

- Three ways in: currents at each scan rate (anodic and cathodic, Δi, or one branch), the CVs themselves (the currents are read at a potential you choose), or Cdl already known
- Cdl as the slope of Δi/2 against the scan rate, the average of the anodic and cathodic slopes as McCrory et al. (2013) do it, with its standard error and R²
- ECSA = Cdl/Cs with Cs = 0.040 mF/cm² (1 M NaOH) or 0.035 mF/cm² (1 M H₂SO₄) as McCrory et al. chose them, or your own value
- Roughness factor and specific ECSA (m²/g) from the geometric area and the catalyst mass; current densities per geometric cm² work too
- Warnings when the line is not straight, misses the origin, or the anodic and cathodic slopes disagree (a Faradaic current in the window)
- Plot of the charging current against scan rate as PNG (300 or 600 dpi), results as CSV, a methods sentence, and the fit in the Graph app; nothing is uploaded

## How to use it

1. **Choose what you have**: The anodic and cathodic currents read at each scan rate, the CVs themselves, or a Cdl you already have.
2. **Enter the charging currents**: Paste scan rate, anodic current and cathodic current (one row per scan rate), or paste the CVs (potential, current, scan rate) and choose the potential to read them at.
3. **Choose the specific capacitance**: Take 0.040 mF/cm² for 1 M NaOH or 0.035 mF/cm² for 1 M H₂SO₄ (McCrory et al. 2013), or type a value measured for your material.
4. **Enter the geometric area**: The area of the electrode (0.196 cm² for a 5 mm disc) gives the roughness factor; add the catalyst mass under More options for the specific ECSA.
5. **Read and export**: Read Cdl, ECSA and the roughness factor, check the plot and the warnings, and copy the results or the methods sentence.

## At a glance

| | |
| --- | --- |
| Formula | \(C_\mathrm{dl}\) = slope of \(\Delta i/2\) against \(\nu\); ECSA = \(C_\mathrm{dl}/C_\mathrm{s}\); RF = ECSA/\(A_\mathrm{geo}\) |
| Cs presets | 0.040 mF/cm² (1 M NaOH), 0.035 mF/cm² (1 M H₂SO₄), McCrory et al. 2013; or your own |
| Input | Currents at each scan rate, whole CVs (read at a chosen potential), or Cdl; A, mA, µA, nA or per cm² |
| Fit | Least squares with an intercept (the Graph app’s linear regression); anodic and cathodic slopes shown |
| Output | Cdl ± SE, ECSA, roughness factor, specific ECSA; plot (PNG), CSV, methods sentence |

## How it works

$$i_\mathrm{c} = C_\mathrm{dl}\,\nu, \qquad \mathrm{ECSA} = \frac{C_\mathrm{dl}}{C_\mathrm{s}}, \qquad \mathrm{RF} = \frac{\mathrm{ECSA}}{A_\mathrm{geo}}$$

**Double-layer capacitance.** In a potential window where no Faradaic process takes place, the current of a CV only charges the double layer, and its size is the capacitance times the scan rate, \(i_\mathrm{c} = C_\mathrm{dl}\,\nu\). McCrory et al. (2013) record CVs in such a window at scan rates from 0.005 to 0.4 V/s, holding the electrode at each vertex for 10 s, plot the anodic and the cathodic charging current at one potential against the scan rate, and take Cdl as “the average of the absolute value of the slope of the linear fits”. The calculator fits a straight line (least squares, with an intercept) to \(\Delta i/2 = (i_\mathrm{a} - i_\mathrm{c})/2\) against \(\nu\). Because least squares is linear in the data, the slope of \(\Delta i/2\) is exactly the average of the anodic slope and the absolute cathodic slope when both are measured at the same scan rates; both are shown, since a large difference between them points to a Faradaic current. With current densities per geometric cm², Cdl comes out per geometric cm². A current in µA against a scan rate in mV/s has its slope in mF.

**From the CVs.** Pasted CVs are split by scan rate; on each, the current at the chosen potential is interpolated linearly between the two points either side of it, on the last rising (anodic) and the last falling (cathodic) sweep. By default the potential is the middle of the window every CV covers.

**ECSA and roughness factor.** The specific capacitance Cs is the capacitance of an atomically smooth surface of the material in the electrolyte; the ECSA is Cdl/Cs, the roughness factor is ECSA divided by the geometric area, and the specific ECSA is ECSA divided by the catalyst mass. McCrory et al. chose 40 µF/cm² in 1 M NaOH and 35 µF/cm² in 1 M H₂SO₄ as typical values of reported metal surfaces, noting that most lay between 22 and 40 µF/cm² in alkaline solution and that the true value may differ by a factor of 3–4, so the roughness factors are believable to about an order of magnitude.

**Limits.** The method assumes a purely capacitive current with one Cs for the whole surface. Pseudocapacitance (surface redox of oxides), a poorly conducting catalyst or support, and Faradaic background currents all distort it, which is why Wei et al. (2019) review it next to other ways of measuring the surface area of oxide electrocatalysts and discuss the uncertainty of each. Use it to compare electrodes of the same material measured the same way, and report Cdl, Cs and the window.

## Worked example: Cdl, ECSA and roughness factor from six scan rates

The built-in example is synthetic, not a measurement: a catalyst film on a 5 mm glassy-carbon disc (0.196 cm²) in 1 M KOH, CVs at 10 to 100 mV/s between 0.90 and 1.00 V vs RHE, and the charging currents read at 0.95 V.

| ν (mV/s) | i_a (µA) | i_c (µA) | Δi/2 (µA) |
| --- | --- | --- | --- |
| 10 | 1.53 | −1.33 | 1.430 |
| 20 | 2.97 | −2.77 | 2.870 |
| 40 | 5.90 | −5.53 | 5.715 |
| 60 | 8.83 | −8.37 | 8.600 |
| 80 | 11.72 | −11.11 | 11.415 |
| 100 | 14.63 | −13.96 | 14.295 |

- **Half the difference.** At 100 mV/s, \(\Delta i/2 = (14.63 + 13.96)/2 = 14.295\ \upmu\mathrm{A}\).
- **Fit the line.** Δi/2 against ν has a slope of 0.14283 µA per mV/s, so \(C_\mathrm{dl} = \mathbf{0.1428\ mF}\) (± 0.0002 mF, R² = 0.99999). The anodic slope is 0.1457 mF and the cathodic −0.1400 mF; their absolute average is the same 0.1428 mF.
- **ECSA.** With Cs = 0.040 mF/cm² (1 M NaOH), \(\mathrm{ECSA} = 0.14283 / 0.040\) \({}= \mathbf{3.571\ cm^2}\).
- **Roughness factor.** \(\mathrm{RF} = 3.571 / 0.196 = \mathbf{18.2}\).
- **Specific ECSA.** With 0.05 mg of catalyst on the disc, \(3.571 \times 10^{-4}\ \mathrm{m^2} / 5 \times 10^{-5}\ \mathrm{g}\) \({}= 7.14\ \mathrm{m^2/g}\).

**From the CVs.** Choose “The CVs” and Example: the six synthetic CVs behind these numbers (anodic capacitance 0.146 mF, cathodic 0.140 mF, a small sloping background and noise) are read at 0.95 V, the middle of the window, giving Cdl = 0.1427 mF and an ECSA of 3.57 cm².

**A published check.** McCrory et al. (2013, Supporting Information, Figure S13) measured a Pt disk in 1 M H₂SO₄: slopes of 0.0725 mF (anodic) and −0.0736 mF (cathodic), Cdl = 0.073 mF, and with Cs = 0.035 mF/cm² an ECSA of 2.1 cm². Under “Cdl already”, 0.07305 mF with the acid value gives 2.087 cm².


## Specific capacitances reported for metal surfaces

The values McCrory et al. (2013) compiled from the literature to choose their general Cs (Supporting Information, Table S1), in µF/cm². Their choice: 40 µF/cm² (0.040 mF/cm²) in 1 M NaOH and 35 µF/cm² (0.035 mF/cm²) in 1 M H₂SO₄.

| Material | Alkaline solution | H₂SO₄ solution |
| --- | --- | --- |
| C | 22 (5 M KOH) | 13–17 (1 M) |
| Co | 27 (1 M NaOH) |  |
| Cu | 130 (1 M NaOH) | 25 (1.8 M), 50 (0.5 M) |
| Mo | 30 (1 M NaOH) | 27 (1 N) |
| Ni | 25 (1 M NaOH), 40 (0.5 M KOH), 30 (31 % KOH), 22 (4 N KOH) | 20 (0.5 M) |
| NiCo | 26 (1 M NaOH) |  |
| NiMoCd | 90 (0.5 M KOH) |  |
| Pt | 60 (1 N KOH), 28 (1 M KOH) | 17 (1 M), 35–45 (1 N), 110 (1 N), 15 (0.1 N) |
| Pt/C | 30 (1 M KOH) |  |
| CuAu |  | 30 (1 M) |
| Stainless steel | 29 (1 M NaOH) |  |

The spread is why an ECSA from Cdl is an estimate: use a Cs measured on a flat sample of your material if you have one, and always state the value.

## Common mistakes with ECSA from Cdl

- **A window with Faradaic current.** Peaks, a sloping background or a line that misses the origin mean the current is not only double-layer charging; choose a narrow window (about 0.1 V) around the open-circuit potential where the CV is rectangular.
- **Only one branch, or the full Δi.** The anodic and cathodic currents each give Cdl; their difference Δi gives 2·Cdl. Use Δi/2 (or the average of the two slopes).
- **Too few scan rates, or too fast.** Use five or more; at high scan rates the uncompensated resistance rounds the CV and lowers the current.
- **Treating Cs as known.** 0.040 and 0.035 mF/cm² are general values; for oxides with pseudocapacitance the ECSA can be far off. Compare like with like and state Cs.
- **Mixing areas.** Cdl from currents in mA gives the ECSA directly; from current densities per geometric cm² it gives the roughness factor.

## References

- McCrory CCL, Jung S, Peters JC, Jaramillo TF. Benchmarking heterogeneous electrocatalysts for the oxygen evolution reaction. *J Am Chem Soc* 2013;135:16977–16987. [doi:10.1021/ja407115p](https://doi.org/10.1021/ja407115p) (method, Cs of 0.040 and 0.035 mF/cm², Table S1 and Figure S13 in the Supporting Information)
- Wei C, Sun S, Mandler D, Wang X, Qiao SZ, Xu ZJ. Approaches for measuring the surface areas of metal oxide electrocatalysts for determining their intrinsic electrocatalytic activity. *Chem Soc Rev* 2019;48:2518–2534. [doi:10.1039/C8CS00848E](https://doi.org/10.1039/C8CS00848E)
- McCrory CCL, Jung S, Ferrer IM, Chatman SM, Peters JC, Jaramillo TF. Benchmarking hydrogen evolving reaction and oxygen evolving reaction electrocatalysts for solar water splitting devices. *J Am Chem Soc* 2015;137:4347–4357. [doi:10.1021/ja510442p](https://doi.org/10.1021/ja510442p)


## Related calculators

- [Tafel slope calculator](https://www.labcanvas.com/tools/tafel-slope-calculator): Tafel slope in mV/dec and the exchange current density from a polarisation curve.
- [Turnover frequency (TOF) calculator](https://www.labcanvas.com/tools/turnover-frequency-calculator): Turnover frequency (TOF) and TON for electrocatalysis (j/nFΓ) or heterogeneous catalysis, with the active sites counted several ways.
- [RHE converter](https://www.labcanvas.com/tools/rhe-calculator): Potentials vs Ag/AgCl, SCE or Hg/HgO converted to the RHE scale, with iR correction and overpotential.
- [All 39 lab calculators](https://www.labcanvas.com/tools/lab-calculators)

## Use this calculator from code or an AI agent

This calculator also answers as JSON, computed by the same code as this page: no key, no account, CORS open. Send the parameters as a query string (numbers may carry units; lists comma-separated) or POST them as JSON to https://www.labcanvas.com/api/tools/ecsa-calculator. An example, with the answer shortened to its first values:

```
GET https://www.labcanvas.com/api/tools/ecsa-calculator?scan_rate=10%2C20%2C40%2C60%2C80%2C100&anodic_current=1.53%2C2.97%2C5.90%2C8.83%2C11.72%2C14.63&cathodic_current=-1.33%2C-2.77%2C-5.53%2C-8.37%2C-11.11%2C-13.96&geometric_area=0.196
```

```json
{
 "ok": true,
 "tool": "ecsa-calculator",
 "inputs": {"scan_rate":{"value":[10,20,40,60,80,100],"unit":"mV/s"},"anodic_current":{"value":[1.53,2.97,5.9,8.83,11.72,14.63]},"cathodic_current":{"value":[-1.33,-2.77,-5.53,-8.37,-11.11,-13.96]}},
 "result": {"cdl":{"label":"Double-layer capacitance Cdl","value":0.1428287671,"unit":"mF"},"cdl_se":{"label":"Standard error of Cdl","value":0.0002019560938,"unit":"mF"}},
 "answer": "Cdl = 0.1428 mF from 6 scan rates (R² = 0.99999); ECSA = 3.571 cm², roughness factor 18.22 with Cs = 0.04 mF/cm² (1 M NaOH, McCrory et al. 2013).",
 "formula": "Cdl = slope of Δi/2 = (i_a − i_c)/2 against ν (least squares; = mean of the anodic and |cathodic| slopes); ECSA = Cdl/Cs; RF = ECSA/A_geo (McCrory et al. 2013, doi:10.1021/ja407115p)",
 "page": "https://www.labcanvas.com/tools/ecsa-calculator",
 "citation": "LabCanvas ECSA calculator, https://www.labcanvas.com/tools/ecsa-calculator"
}
```

Parameters:

- `scan_rate` (number[], mV/s): Scan rates (mV/s), one per measurement.
- `anodic_current` (number[]): Anodic charging current at one potential for each scan rate, in current_unit (or Δi when cathodic_current is left out and delta = true).
- `cathodic_current` (number[]): Cathodic charging current at the same potential (negative, or positive magnitudes).
- `delta` (boolean, default false): true: anodic_current holds Δi = i_a − i_c (no cathodic_current).
- `current_unit` (string, default uA: A | mA | uA | nA | mA/cm2 | uA/cm2): Unit of the currents; per cm² for current densities per geometric area.
- `cdl` (number, mF): Cdl already known (mF, or mF per geometric cm² with cdl_per_area), instead of the currents.
- `cdl_per_area` (boolean, default false): cdl is per geometric cm².
- `specific_capacitance` (number, mF/cm², default 0.04): Cs (mF/cm²): 0.040 in 1 M NaOH, 0.035 in 1 M H₂SO₄ (McCrory et al. 2013), or a value for your material.
- `geometric_area` (number, cm²): Geometric electrode area (cm²), for the roughness factor.
- `catalyst_mass` (number, mg): Catalyst mass on the electrode (mg), for the specific ECSA in m²/g.

All calculators: https://www.labcanvas.com/api/tools · OpenAPI 3.1: https://www.labcanvas.com/api/tools/openapi.json · MCP tool: `calc_ecsa` (LabCanvas MCP server).

## Questions

### How do you calculate ECSA from cyclic voltammetry?

Record CVs at five or more scan rates in a narrow window with no Faradaic current, read the anodic and cathodic current at the same potential, and plot Δi/2 = (i_a − i_c)/2 against the scan rate. The slope is the double-layer capacitance Cdl; divide it by the specific capacitance Cs to get the ECSA: ECSA = Cdl/Cs.

### What specific capacitance should I use for ECSA?

A value measured on a flat surface of your material, if you have one. Otherwise most papers use the general values McCrory et al. (2013) chose: 0.040 mF/cm² in 1 M NaOH and 0.035 mF/cm² in 1 M H₂SO₄. Reported values span about 20–130 µF/cm², so state the one you used.

### Why use Δi/2 and not Δi?

The anodic and cathodic charging currents are each Cdl·ν, so their difference is 2·Cdl·ν. The slope of Δi/2, which equals the average of the anodic and absolute cathodic slopes, is Cdl. Using Δi doubles the ECSA.

### What potential window and scan rates should I use?

A window of about 0.1 V where the CV is rectangular (no redox peaks), usually around the open-circuit potential, and scan rates from a few mV/s up to about 100–400 mV/s. McCrory et al. used 0.005 to 0.4 V/s and held the electrode at each vertex for 10 s.

### What is the roughness factor?

The ECSA divided by the geometric area of the electrode: how many times larger the electrochemically active area is than the footprint. An ECSA of 3.57 cm² on a 0.196 cm² disc is a roughness factor of 18.2.

### How do I normalise activity by ECSA?

Divide the current by the ECSA instead of the geometric area: the specific activity j_ECSA = I/ECSA. Compare specific activities only between catalysts whose ECSA was measured the same way with the same Cs.

### Can I get Cdl from impedance instead?

Yes. McCrory et al. also fitted impedance spectra in the non-Faradaic region with a simplified Randles circuit and got the same Cdl for a Pt disk (0.075 mF against 0.073 mF from CV). Enter that Cdl under “Cdl already”.

### Is the ECSA from Cdl accurate for oxides?

It is an estimate. Pseudocapacitance, conductivity and the choice of Cs can move it by a factor of several, so use it to compare similar electrodes measured the same way, and report Cdl and Cs with it.