Mott–Schottky analyzer: flat-band potential and donor density
A Mott–Schottky plot is 1/C² against the applied potential, with C the space-charge capacitance per unit area. In the depletion region it is a straight line, 1/C² = 2/(e·ε·ε₀·N)·(E − E_fb − kT/e) for an n-type semiconductor, so the flat-band potential is the x-intercept minus kT/e (25.7 mV at 25 °C) and the donor density is N_D = 2/(e·ε·ε₀·slope); a negative slope means p-type, with E_fb = x-intercept + kT/e. Paste capacitance against potential (one or several frequencies) and the analyzer fits the straight part, gives E_fb and N with standard errors, and converts E_fb to the RHE scale.
- What it does
- Fits a straight line to 1/C² against potential over the linear (depletion) region and gives the flat-band potential and the donor or acceptor density for each frequency, with standard errors.
- Formula
- Example
- The built-in synthetic n-type film (ε = 86) at 1 kHz: the line from 0.077 to 0.977 V vs RHE has a slope of 8.525 × 10¹⁰ cm⁴ F⁻² V⁻¹ and meets the axis at 0.0748 V, so E_fb = 0.0748 − 0.0257 = 0.0491 V vs RHE and N_D = 1.92 × 10¹⁹ cm⁻³.
Loading Mott–Schottky analyzer…
At a glance
| Model | |
|---|---|
| Gives | E_fb ± SE, N_D or N_A ± SE, type, slope, region, R²; per frequency |
| Fit | Least squares over the linear region (automatic: longest run without significant curvature; or typed) |
| Input | E with C (per cm² or whole electrode), 1/C², or Z″ with the frequency; optional frequency column |
| Constants | CODATA 2018 (NIST): e, k, ε₀ |
| Output | Mott–Schottky plot (PNG 300/600 dpi), CSV, methods sentence, Graph app |
| Runs in | Your web browser; nothing is uploaded |
| Price | Free, no account needed |
What it does
How to use the mott–Schottky analyzer
- Paste or drop your dataColumns: potential and capacitance, with a frequency column if you measured several frequencies (rows one under another). A header such as E (V vs Ag/AgCl), C (µF/cm²), f (Hz) gives the units; without one, choose what the second column holds.
- Enter the semiconductor and the electrodePick the material for ε or type ε, and enter the electrode area if the capacitance is for the whole electrode.
- Check the frequency and the linear regionChoose the frequency to report and look at the plot: keep the straight part of 1/C², away from the bend near E_fb and from the high-bias end.
- Choose the potential scaleKeep the measured scale, or pick the reference electrode and the pH to report E_fb against RHE.
- Read and exportRead E_fb, N and the type, compare the frequencies, and copy the results, the methods sentence or the plot.
How it works
The Mott–Schottky equation. At a semiconductor–electrolyte junction under depletion, the space-charge layer behaves as a capacitor whose thickness grows with the band bending, so
What the analyzer computes. It converts every row to the capacitance per cm² (dividing by the area when the capacitance is for the whole electrode; from impedance as
(minus for n-type, plus for p-type, the type from the sign of
The linear region. Near
Frequency. The capacitance of a real electrode is usually measured at several frequencies (for example 0.5, 1 and 2 kHz). If the space-charge capacitance is what you measure, the lines meet the axis at the same potential, though the slopes may differ; when E_fb moves with the frequency, the result is uncertain and the frequency should be reported. The analyzer fits every frequency and lists them side by side.
RHE scale. E(RHE) = E + E°(ref) + (ln 10·RT/F)·pH, with the reference electrodes and values of the RHE converter. The slope of 1/C² does not change; only the potentials shift.
Worked example: an n-type film measured at three frequencies
The built-in example is synthetic, not a measurement: an n-type film with ε = 86 (the rutile value of Parker 1961, perpendicular to the c axis), N_D = 2 × 10¹⁹ cm⁻³ and E_fb = −0.950 V vs Ag/AgCl (saturated KCl), measured at 0.5, 1 and 2 kHz in an electrolyte of pH 14 at 25 °C, from −1.100 to −0.050 V in 25 mV steps. To make it realistic, the curve is rounded near E_fb, a 100 µF/cm² Helmholtz layer is in series, the capacitance falls slightly with frequency (C ∝ f^−0.03), and there is 0.4 % noise. The capacitance is per cm², so no area is needed.
- Convert to RHE.
. - Take 1/C². At −0.500 V vs Ag/AgCl and 1 kHz, C = 5.0511 µF/cm², so
. - Fit the straight part. At 1 kHz the automatic region runs from 0.077 to 0.977 V vs RHE (37 points): slope
cm⁴ F⁻² V⁻¹, intercept cm⁴ F⁻², R² = 0.99936. - Flat-band potential.
; the slope is positive, so n-type, and vs RHE (−0.978 V vs Ag/AgCl). - Donor density.
.
| Frequency | E_fb (V vs RHE) | N_D (cm⁻³) | R² |
|---|---|---|---|
| 500 Hz | 0.0494 | 1.99 × 10¹⁹ | 0.99923 |
| 1 kHz | 0.0491 | 1.92 × 10¹⁹ | 0.99936 |
| 2 kHz | 0.0506 | 1.84 × 10¹⁹ | 0.99931 |
The three lines meet the axis within 1.5 mV of each other while the slopes differ by 8 %: the dispersion changes N_D, not E_fb. The fitted E_fb is 28 mV below the true 0.077 V vs RHE, because the Helmholtz layer in series and the rounding near E_fb both bend 1/C². That is typical: a Mott–Schottky flat-band potential carries an uncertainty of some tens of millivolts beyond its standard error, so state the frequency, the region fitted and ε with the result.
Relative permittivity ε of common semiconductors
N is inversely proportional to ε, so the value you use matters as much as the slope. These are static values of single crystals near room temperature, each from the paper cited; films, nanostructures and porous or doped oxides can differ a lot, and for many oxides used as photoelectrodes the published values spread widely. Use a value measured for your material if you can, and cite it.
| Material | ε | Note | Source |
|---|---|---|---|
| Si | 11.7 | 11.7 ± 0.2 at 1 MHz | Dunlap & Watters 1953 |
| GaAs | 13.09 | 12.35 × (1 + 2.01 × 10⁻⁴ K⁻¹ × 298.15 K) | Strzalkowski et al. 1976 |
| CdTe | 11.01 | 10.31 × (1 + 2.27 × 10⁻⁴ K⁻¹ × 298.15 K) | Strzalkowski et al. 1976 |
| ZnSe | 9.25 | 8.80 × (1 + 1.71 × 10⁻⁴ K⁻¹ × 298.15 K) | Strzalkowski et al. 1976 |
| TiO₂, rutile ⊥ c | 86 | a direction, 300 K | Parker 1961 |
| TiO₂, rutile ∥ c | 170 | c direction, 300 K | Parker 1961 |
Strzalkowski et al. give ε extrapolated to 0 K and a linear temperature coefficient λ (valid from 100 to 300 K); the values above are
Common Mott–Schottky mistakes
- Capacitance of the whole electrode used as if per cm². N scales with 1/A²: a 0.2 cm² electrode read as 1 cm² gives N 25 times too high. Enter the area, or the capacitance per cm².
- Forgetting kT/e. The x-intercept is E_fb + kT/e for n-type (E_fb − kT/e for p-type); at room temperature the difference is 25.7 mV.
- Fitting the bend. Points near E_fb and at high bias are not on the depletion line; including them moves the intercept.
- One frequency, no check. If E_fb changes with the frequency, the capacitance is not only the space charge’s (surface states, roughness, a porous film); report the frequency or the spread.
- Mixing potential scales. Convert to RHE (or state the reference) before comparing E_fb with band positions or other papers.
References
- Gelderman K, Lee L, Donne SW. Flat-band potential of a semiconductor: using the Mott–Schottky equation. J Chem Educ 2007;84:685. doi:10.1021/ed084p685
- Bard AJ, Faulkner LR. Electrochemical Methods: Fundamentals and Applications, 2nd ed. Wiley; 2001, section 18.2 (semiconductor electrodes). ISBN 978-0-471-04372-0.
- Tiesinga E, Mohr PJ, Newell DB, Taylor BN. CODATA recommended values of the fundamental physical constants: 2018. Rev Mod Phys 2021;93:025010. doi:10.1103/RevModPhys.93.025010 (NIST: physics.nist.gov/cuu/Constants)
- Dunlap WC, Watters RL. Direct measurement of the dielectric constants of silicon and germanium. Phys Rev 1953;92:1396–1397. doi:10.1103/PhysRev.92.1396
- Strzalkowski I, Joshi S, Crowell CR. Dielectric constant and its temperature dependence for GaAs, CdTe, and ZnSe. Appl Phys Lett 1976;28:350–352. doi:10.1063/1.88755
- Parker RA. Static dielectric constant of rutile (TiO₂), 1.6–1060 °K. Phys Rev 1961;124:1719–1722. doi:10.1103/PhysRev.124.1719
Frequently asked questions
How do you calculate the flat-band potential from a Mott–Schottky plot?
Plot 1/C² (C per unit area) against the potential, fit a straight line to the linear part and find where it meets the potential axis, E₀ = −intercept/slope. For an n-type semiconductor (positive slope) the flat-band potential is E₀ − kT/e; for p-type (negative slope) it is E₀ + kT/e. kT/e is 25.7 mV at 25 °C.
How do I calculate the donor density from the Mott–Schottky slope?
N_D = 2/(e·ε·ε₀·slope), with the slope of 1/C² against E in cm⁴ F⁻² V⁻¹, ε the relative permittivity, ε₀ = 8.854 × 10⁻¹⁴ F/cm and e = 1.602 × 10⁻¹⁹ C; N_D comes out in cm⁻³. If C is the capacitance of the whole electrode, divide also by A² (A in cm²). A slope of 8.5 × 10¹⁰ cm⁴ F⁻² V⁻¹ with ε = 86 gives 1.9 × 10¹⁹ cm⁻³.
Does a positive or negative slope mean n-type or p-type?
A positive slope of 1/C² against potential means n-type (donors): anodic bias deepens the depletion layer. A negative slope means p-type (acceptors). The analyzer reads the type from the sign and reports N_D or N_A.
Which frequency should I use for Mott–Schottky?
Measure at several frequencies in the range where the capacitance is that of the space charge, often around 0.5–10 kHz, and check that the flat-band potential does not depend on the frequency. Paste them all with a frequency column: the analyzer fits each one and compares them.
What dielectric constant should I use?
The static relative permittivity of your semiconductor, ideally measured for the same kind of material. The table on this page gives referenced single-crystal values (Si 11.7, GaAs 13.1, rutile TiO₂ 86 or 170); thin films and nanostructures can differ, so state the value and its source with your result.
Why is my Mott–Schottky plot not linear?
Near the flat-band potential the depletion approximation fails, and at high bias surface states, a Helmholtz layer in series, deep depletion or a thin film fully depleted bend the plot. A rough or porous electrode also gives frequency-dependent capacitance. Fit only the straight part and report the range.
How do I convert the flat-band potential to the RHE scale?
E(RHE) = E(ref) + E°(ref) + 0.0592 V × pH at 25 °C: for Ag/AgCl in saturated KCl (0.199 V) at pH 14, add 1.027 V. Choose the reference and the pH in step 4, or use the RHE converter.
Can I use the capacitance from an impedance fit?
Yes: paste the space-charge capacitance from your equivalent-circuit fit against potential. If you only have the imaginary impedance at one frequency, paste Z″ with the frequency and the analyzer takes C = 1/(2πf|Z″|), which assumes a simple series RC.
Link to this tool
Using it in a protocol, lab wiki or course page? Copy a link or citation.
<a href="https://www.labcanvas.com/tools/mott-schottky-analyzer">Mott–Schottky analyzer</a> (LabCanvas)LabCanvas. Mott–Schottky analyzer [online tool]. https://www.labcanvas.com/tools/mott-schottky-analyzerPlot the Mott–Schottky data for your paper
The LabCanvas Graph app draws the Mott–Schottky plot with the fitted line and the flat-band potential, from the same analysis, ready to restyle and size for a journal. Your data from this page open in it.
Open the Mott–Schottky graph